Next Article in Journal
Explicit Lump Solitary Wave of Certain Interesting (3+1)-Dimensional Waves in Physics via Some Recent Traveling Wave Methods
Next Article in Special Issue
Solidification Microstructures of the Ingots Obtained by Arc Melting and Cold Crucible Levitation Melting in TiNbTaZr Medium-Entropy Alloy and TiNbTaZrX (X = V, Mo, W) High-Entropy Alloys
Previous Article in Journal
Energy Use of Flux Salt Recovery Using Bipolar Membrane Electrodialysis for a CO2 Mineralisation Process
Previous Article in Special Issue
A Study on the Hall–Petch Relationship and Grain Growth Kinetics in FCC-Structured High/Medium Entropy Alloys
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Mechanical Properties and Corrosion Resistance of NbTiAlSiZrNx High-Entropy Films Prepared by RF Magnetron Sputtering

1
State Key Laboratory of Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083, China
2
School of Mechanical Engineering, Qinghai University, Xining 810016, China
3
Qinghai Provincial Engineering Research Center of High Performance Light Metal Alloys and Forming, Xining 810016, China
4
Qinghai Provincial Key Laboratory of New Light Alloys, Xining 810016, China
5
University of Sheffield, Sheffield S37GE, UK
6
School of Materials Science, Shanghai DianJi University, Shanghai 201306, China
*
Author to whom correspondence should be addressed.
These authors contributed equally: Q. Xing, H. Wang and M. Chen.
Entropy 2019, 21(4), 396; https://doi.org/10.3390/e21040396
Submission received: 28 February 2019 / Revised: 5 April 2019 / Accepted: 8 April 2019 / Published: 13 April 2019
(This article belongs to the Special Issue High-Entropy Materials)

Abstract

:
In this study, we designed and fabricated NbTiAlSiZrNx high-entropy alloy (HEA) films. The parameters of the radio frequency (RF) pulse magnetron sputtering process were fixed to maintain the N2 flux ratio at 0%, 10%, 20%, 30%, 40%, and 50%. Subsequently, NbTiAlSiZrNx HEA films were deposited on the 304 stainless steel (SS) substrate. With an increasing N2 flow rate, the film deposited at a RN of 50% had the highest hardness (12.4 GPa), the highest modulus (169 GPa), a small roughness, and a beautiful color. The thicknesses of the films were gradually reduced from 298.8 nm to 200 nm, and all the thin films were of amorphous structure. The electrochemical corrosion resistance of the film in a 0.5 mol/L H2SO4 solution at room temperature was studied and the characteristics changed. The HEA films prepared at N2 flow rates of 10% and 30% were more prone to corrosion than 304 SS, but the corrosion rate was lower than that of 304 SS. NbTiAlSiZrNx HEA films prepared at N2 flow rates of 20%, 40%, and 50% were more corrosion-resistant than 304 SS. In addition, the passivation stability of the NbTiAlSiZrNx HEA was worse than that of 304 SS. Altogether, these results show that pitting corrosion occurred on NbTiAlSiZrNx HEA films.

1. Introduction

Improving corrosive resistance and mechanical properties is an important part of alloy thin film research [1,2,3,4,5,6,7]. The reasonable design of alloy thin films is the premise for the preparation of excellent films [8,9,10], whereas the proper preparation of the target and selection of the appropriate substrate are prerequisites in their preparation [11,12]. High-entropy alloys (HEAs) have excellent performance due to their high mixing entropy effects, microstructure strengthening, sluggish diffusion, cocktail effects, and structural stability effects [13,14,15,16]. Feng et al. reported that the mechanical property of FeCoNi(AlSi)x is affected by the chemical short-range order in alloys [17]. Adding Co and Gd can affect the microstructures and properties of FeSiBAlNi HEAs [18]. The oxide can improve the tensile strength of CrMnFeCoNi HEAs [19]. Besides composition, fabrication methods can also affect the microstructure and mechanical properties of HEAs [20,21]. Magnetron sputtering and laser cladding are two of the most important methods for preparing HEA coatings [22,23,24,25,26,27,28]. Both N2 flow rate and substrate bias affect hardness, the elastic modulus, and corrosive resistance of HEA coatings. Hsueh et al. prepared a (AlCrSiTiZr)(100-x)Nx coating (amorphous) by magnetron sputtering on the surface of a 6061 aluminum alloy plate. The researchers changed the conditions of nitrogen flow ratio (RN) to increase the (AlCrSiTiZr)100-xNx thin film content to 30%, which was deposited on the 6061 aluminum alloy and carbon steel substrate, thereby optimizing the mechanical properties and corrosive resistance of HEA thin films. Hardness of the HEA (AlCrSiTiZr)(100-x)Nx coating (amorphous) reaches 34 GPa [7], while that of NiCrAlCoMo HEA thin films was 1000 HV. The films were prepared by magnetron sputtering on a carbon steel substrate, and contained more intermetallic compounds. Its friction coefficient was low at 0.6, and it had good wear resistance. The hardness of the magnetron sputtering (AlCrNbSiTiV)N HEA film was 41 GPa. The hardness of the (AlCrTiZr)Si7.9N film was 34 GPa, and the oxidation resistance is excellent [29]. Hardness of the HEA film (AlCrTiZr) N0.6C0.2 was 32 GPa, and the creep rate was low at 1.1 × 10−4 s−1. The corrosive resistance was excellent [30]. The AlxFeCrCoNiCu HEA coating prepared on a steel substrate by magnetron sputtering has good anti-corrosive properties [31]. Sheng et al. [32] used direct-current (DC) bias magnetron sputtering amorphous NbTiAlSiNx films with high hardness and modulus. The microstructures of the films are amorphous, and the microstructures are transformed into crystal structures at temperatures above 1000 °C. Sheng et al. [23] reported that amorphous NbTiAlSiWxNy HEA films have high hardness and modulus, and are thermally stabile up to 700 °C, whereas the films transformed into crystal structures at temperatures greater than 1000 °C. Xing et al. [33] reported that NbTiAlSiZrNx HEA films sputtered by direct current power had good thermal stability at 600 °C. The Cr6Fe6V6Ta42W40 multicomponent alloy film exhibited great solar absorption at room temperature [34]. The (Al0.5CrFeNiTi0.25)Nx HEA nitride films achieved higher hardness and Young’s modulus than as-cast (Al0.5CrFeNiTi0.25)Nx bulk alloys [35]. These results indicated that HEA films have potential application on protective coatings to improve the hardness and corrosion resistance of knives and cutting tools.
TiAlN and ZrN films have been widely used as protective coating. The NbTiAlSi system HEA films have been reported to possess high hardness and modulus [23,32,33]. CoCrFeNiAl0.3 films fabricated by RF sputtering demonstrate better corrosion resistance than in 3.5 wt. % NaCl solution. The hardness of CoCrFeNiAl0.3 can reach 11.5 GPa. Moreover, the addition of non-metallic elements has been shown to be an effective means for improving the properties of HEAs [36]. In this regard, we prepared a new five primary element NbTiAlSiZr HEA of equimolar content, and then used the processing methods and RN conditions—which were different from those previously reported in [25], using the radio frequency (RF) magnetron sputtering equipment, processes, and other parameters of fixed technologies—to prepare the NbTiAlSiZrNx HEA thin films under different RN values (0%, 10%, 20%, 30%, 40%, and 50%) and gases (i.e., RN is the only process variable). Then the roughness, color, and performance of these thin films were studied. Spectroscopic analysis showed that the NbTiAlSiZrNx HEA thin film chemical composition was feasible, the preparation process was appropriate, the phase structure was amorphous, and the performance testing indicators met the requirements. Our data show that with increasing RN, the film’s performance indicators, surface color, and roughness could be changed.

2. Materials and Methods

2.1. Design and Fabrication of NbTiAlSiZrNx HEA Thin Films

2.1.1. Design of NbTiAlSiZrNx HEA Films

According to the theory and design of HEAs, as well as the results of previous studies on NbTiAlSiZr HEA synthesis, the elemental composition of Nb:Ti:Al:Si:Zr was 20:20:20:20:20.
According to Equations (1) and (2), we calculated the radius difference of the constituent atoms as follows:
δ = i = 1 n c i ( 1 r i r ¯ ) 2
r ¯ = i = 1 n c i r i
where r ¯ is the average radius of alloying elemental atoms and ri is the radius of the ith elemental atom (Table 1).
The calculated results (δ = 1.1% < 6.5%) reflected a change in the atomic radius of the primary element after HEA formation.
According to Equation (3), we calculated the mixing enthalpy ΔSmix of the primary elements Nb, Ti, Al, Si, and Zr as follows:
Δ S m i x = R i = 1 n ( c i ln c i )
where R = 8.314 J/mol·K is the gas constant, n is the primary element number of the alloy, and ci is the ith primary element content (%).
The calculated results (ΔSmix = 1.566 R) failed to meet the thermodynamic conditions (1 R < ΔSmix < 1.5 R) of the solid HEA. These results suggest that an amorphous or compound HEA was formed. The NbTiAlSiZrNx HEA film had a thickness of 200–300 nm and a surface roughness of 0.2–0.4 nm.

2.1.2. Preparing the NbTiAlSiZrNx HEA Film

The commonly used methods for preparing HEA films are co-sputtering with multi-target and sputtering by HEA target. The compositional deviation of the latter method is less than the former. In this regard, we sputtered the HEA target to form HEA films. According to the constituent elements of the NbTiAlSiZr HEA, the HEA target was prepared using a hot isostatic pressing process. In brief, different NbTiAlSiZrNx HEA films were prepared using a JGP-450 single-target RF magnetron sputtering instrument with parameters as follows: a target base distance of 60 mm; a vacuum pressure of 6 × 10−4 Pa; a sputtering pressure of 0.6 Pa; an Ar gas flow rate constant of 25 sccm; a voltage of 600 V; a current of 180 mA; a sputtering power of 120 W; a pulse frequency of 13.56 MHz; and nitrogen flow rates of 0, 3, 6, 11, 17, and 25 sccm, respectively (i.e., corresponding to nitrogen flow rates of 0, 10, 20, 30, 40, and 50%, respectively), and a single sample sputtering time of 60 min. The elemental components of the HEA film were identified by energy dispersive X-Ray spectroscopy (EDX) after sputtering. For the potential compositional deviation, we prepared two solutions: (1) using assisted targets to supplement the lack elements; and (2) adjusting the composition of the alloy target. The elemental components of NbTiAlSiZr HEA films are listed in Table 2. According to Table 2, the maximum element deviation is only 1 at. % after testing (Al: 21.00 at. %). Because the accuracy range of EDX measurements is not less than 1 at. %, the composition of HEA film was uniform and did not need further compositional adjustment in this work.

2.2. Characterization of the NbTiAlSiZrNx HEA Thin Film Method

2.2.1. Assessment of Film Thickness

The film cross-sections were observed under an Auriga model field emission scanning electron microscope (Carl Zeiss, Jena, Germany). Working distance (WD) was 9 mm and the extra high tension (EHT) was 15 kV.
Based on our experience with alloys, we opted to use N-type single-side polished monocrystalline silicon (100) with a purity of 99.999% and a size of φ 50.8 × 0.5 mm as the substrate. The size of the single crystal sodium chloride ([100] crystal plane) was 20 × 20 × 2 mm, whereas that of the single-side polished 304 stainless steel (304 SS) was 10 × 10 × 2 mm. Single crystal silicon ([100] crystal face) substrate films are conducive to tests of phase structure, whereas single crystal sodium chloride ([100] crystal face) substrate films are conducive to transmission analyses of the phase structure. In addition, 304 stainless steel (304 SS) substrate films are conducive to testes of corrosion resistance. An ultrasonic BG-01 model cleaner was used to clean the substrates, followed by drying.

2.2.2. Assessment of the Film Surface

The film surface was observed under a Bruker multi-mode 8 SPM atomic force microscope, and the film surface roughness was measured in the Scan Asyst smart imaging mode. The size of scanning range was 5 × 5 μm2.

2.2.3. Assessment of Film Hardness

The displacement-load curves of the thin film were measured with a nano-indentor, and then the hardness and modulus were calculated. The working parameters were as follows: tan effective range of 100–200 nm, a press-in depth of 1 μm, a press-in rate of 0.05 nm/s, and Poisson’s ratio of 0.25.

2.2.4. Thin Film Corrosion Resistance

Electrochemical potentiometric electrode polarization tests were performed on thin film-coated 304 SS substrates using the PARSTAT Model 2273 electrochemical workstation at room temperature. The saturated calomel electrode served as the reference electrode, and the platinum electrode served as the auxiliary electrode. The thin film-coated 304 SS substrate was the working electrode, and the etching solution was 0.5 mol/L H2SO4. The sample that was submerged into the corrosive solution was connected to a wire, and all other bare surfaces excluded from the test surface were coated with silica gel. The open-circuit potential of the sample was measured until it stabilized, followed by scanning of the potential. The range of the potential scan was −1.0–1.5 V, scanning speed was 1 mV/s, and samples were etched for 2500 s in 0.5 mol/L H2SO4 solution.

2.2.5. Thin Film Crystal Structure Test

The surface morphology of the thin film was observed under a Technic G2 F-30 S-TWIN transmission electron microscope (TEM). The sample, with a size of 5 × 5 mm, was coated onto the sodium chloride substrate. The sodium chloride substrate was dissolved in deionized water to obtain a thin film for observation using TEM. The sample was measured with an O8DISCOVER high-resolution diffractometer. The sample size was 10 × 10 mm, and EHT was 300 kV.
The crystal structure of the thin film was determined using a Dmax X-ray diffractometer and a Cu Kα (40 kV, 20 mA) source. The X-ray grazing angle was 1°, the diffraction angle 2θ range was 20–80°, and the scanning speed was 3 °/s.

3. Results

3.1. Assessment of Film Thickness

As the RN increased from 20% to 50% during the preparation process, the thickness decreased from 298.8 nm to 200 nm (Figure 1 and Figure 2).

3.2. Assessment of the Film Surface

The surface of NbTiAlSiZrNx HEA films was beautiful, and various base films created different colors. With increasing RN, the color of the same base film changed its hue and saturation (Figure 3a–e), whereas film colors had good decorative effects. Surface roughness of NbTiAlSiZrNx HEA films increased with increasing RN from 10 to 50%. However, the non-monotonicity increased from 0.275 nm to 0.365 nm. The roughness was high at RN = 30%. The surface roughness was not uniform across the various regions of the film (Figure 3 and Figure 4).

3.3. Assessment of Film Hardness

The displacement-load curves of various specimens are reported. The increasing trends of the load-displacement curves of the specimens with different RN were similar (Figure 5a). From load-displacement curves, we calculated the loading energy during the lording process using following equation:
W = P d h
where Wload is the loading energy, h is the displacement, and P is the load on sample. The Wload versus RN curve are exhibited in Figure 5b. Wload represent the energy required for the deformation of HEA films. As is shown in Figure 5b, the Wload increased from 5.13 × 10−7 mJ to 5.69 × 10−7 mJ when RN ranged from 10–30%, the Wload slightly decreased to 5.61 × 10−7 mJ when RN was 40%, then increased to 6.18 × 10−7 mJ when RN was 50%. Resistance to external deformation became stronger with the increasing nitrogen content in NbTiAlSiZrNx HEA films. Figure 5c shows the hardness-displacement curves of the specimens with different RN, indicating that the hardness gradually increased with the increasing indentation depth in the films. The hardness reached a plateau when the displacement was deeper than 40 nm. To avoid the effect of substrate, we calculated the average hardness and modulus in the depth range of 50–100 nm [37]. The surface hardness and modulus of each sample were high, which increased gradually with increasing RN during preparation, and the hardness had a similar trend (Figure 5d). The lowest hardness of the sample with RN of 10% was 9.7 GPa, whereas the highest modulus of sample with RN of 50% was 184.5 GPa.

3.4. Thin Film Corrosion Resistance

The corrosion degree of the different thin films, which were prepared with various RN conditions, was different. Corrosion of the sample prepared with 10% RN was slight, and it had almost no pitting corrosion in the 0.5 mol/L H2SO4 solution (Figure 6f). Non-uniform local pitting corrosion occurred in samples prepared under conditions of RN = 20–50% (Figure 6g–j). However, the most significant non-uniform local pitting corrosion occurred in samples prepared under conditions of RN = 20%. With the increase in RN, the number of pits increased, but the maximum size of the corrosion pits decreased (Figure 7). The corrosion potential of 304 SS was approximately −0.25 V, and the corrosion current Icorr was approximately 10−7 A/cm2. The corrosion potential Ecorr with RN 10% and RN 30% of the samples was approximately −0.3 V, and the corrosion current Icorr was approximately 10−8 A/cm2. The corrosion potential Ecorr of the samples with 20%, 40%, and 50% RN were higher than those of 304 SS, but the corrosion current Icorr was lower than that of 304 SS. The self-corrosion potential and self-corrosion current size at RN = 10% and RN = 30% were similar, and the polarization rate was identical. The self-corrosion potential and corrosion current for the RN = 20% sample were larger, but the polarizability was lower than the RN = 50% sample. The self-corrosion potential of RN = 50% sample was moderate, the self-corrosion current was high, and the polarization rate was low (Figure 8). The passivation interval was not obvious after comparing the NbTiAlSiZrNx HEA thin film with the 304 SS sample, and the passivation interval department start potential and current of NbTiAlSiZrNx HEA thin film were larger than those of the 304 SS sample. The passivation layer breakdown voltage of NbTiAlSiZrNx HEA film samples was lower than that of the 304 SS sample.

3.5. Assessment of the Thin Film’s Crystal Structure

The microstructure of the polycrystalline phases, such as the grain boundary, were not observed by transmission electron microscopy. The electron diffraction patterns were of diffracting rings, rather than single crystal diffraction spots array of the polycrystalline phases (Figure 9). The X-ray diffraction lines of each sample showed amorphous phase diffraction characteristics. The low and wide protuberant peaks on each line were not the normal diffraction peaks in the NbTiAlSiZrNx HEA films, which may have been caused by inclusions in the films (Figure 10). The results indicate that the different RN samples in the preparation process all had an amorphous structure.

4. Discussion

4.1. Preparation of NbTiAlSiZrNx HEA Films Using N2 Magnetron Sputtering and Thin Film Forming Effect

NbTiAlSiZrNx HEA thin films with an optimal thickness, roughness, and hardness, as well as corrosion resistance, were designed to meet design requirements. The N content in NbTiAlSiZrNx HEA thin films changed with RN during preparation. The test results of NbTiAlSiZr HEA films show that preparing NbTiAlSiZr HEA with proper conditions was feasible. RF magnetron sputtering under the different RN conditions of the process were also feasible to reach the preparation requirements of the NbTiAlSiZrNx HEA thin film.
RN significantly affected the thickness, surface roughness, and color of the prepared thin films in the process. According to the existing theory, increasing the RN value can increase the plasma density near the cathode target and the sputtering yield, so that the sputtered metal atoms are more likely to collide with each other during movement, which reduces the ratio reaching the deposition area on the substrate. By contrast, reducing the kinetic energy of the sputtered atoms colliding with the deposition surface above the substrate and weakening the ratio of strongly adsorbed and bonded to the deposition layer, therefore, need to reduce the thickness of the deposited film during processing. After the plasma density increased, the increased temperature enhanced the thermal radiation on the substrate’s deposition surface. As a result, the thermal kinetic energy of some deposition atoms is increased and then desorbed and volatilized from the deposition surface, thereby reducing the deposition growth rate of the thin film and reducing the accumulation of non-uniform deposition volume during processing. Therefore, the deposited thin film thickness and surface roughness were decreased.
The sputtered metal atoms and N2 crashed and were decomposed by N atoms and N+ ions of the ionization under a high degree of vacuum and the high temperature. However, that collision and decomposition on the surface of the initial substrate deposition layer were not uniform. The adsorbed atoms on the surface had been volatized, thereby making the surface roughness and atomic distribution of the sample not uniform. Moreover, the uniformity of color on the surface of the thin film sample was altered, and different sample surfaces were affected by different degrees of color.

4.2. Organizational Structure of the NbTiAlSiZrNx HEA Thin Film

Using TEM, we observed no apparent grain boundaries in the thin film samples. The electron diffraction patterns showed amorphous diffraction patterns, and the X-ray diffraction patterns showed no evidence of crystal diffraction, indicating that the prepared NbTiAlSiZrNx HEA thin film was amorphous in structure. N atoms were dispersed in the film and mixed with various metal atoms to form an amorphous phase.

4.3. Performance of the NbTiAlSiZrNx HEA Thin Film

The hardness and modulus of NbTiAlSiZrNx HEA thin film samples increased with the increase of RN during preparation. Hardness of the 50% RN sample reached the highest value at 12.4 GPa, and the modulus reached the highest value at 169 GPa. If the sample had a high hardness, then it had a high wear resistance. The NbTiAlSiZrNx HEA thin film had a beautiful color, which can be used for decorative purposes. However, its roughness affects the decorative effect. The surface roughness of the NbTiAlSiZrNx HEA thin film was small, and it decreased with the decreasing of RN. The difference of RN during thin film preparation caused differences in the hardness, surface color, and roughness of the film.
The N2 flow rate in the 0.5 mol/L H2SO4 solution increased during the process. The electrochemical corrosion resistance of the NbTiAlSiZrNx HEA thin film in 0.5 mol/L H2SO4 solution changed. The corrosion rate of the entropy alloy film was more likely to be eroded compared with 304 SS when HEA thin film with 10% RN and 30% RN compared with 304 SS. However, the corrosion rate of NbTiAlSiZrNx HEA film with RN 20%, 40%, and 50% was lower than that of 304 SS. Furthermore, the passivation stability of the NbTiAlSiZrNx HEA was worse than that of 304 SS. The thin film with a N2 flow ratio of 40% had a low polarizability and high corrosion resistance. The film with an N2 flow ratio of 30% had a high polarizability and low corrosion resistance. No pitting corrosion occurred in the thin film with a N2 flow rate of 10%. The pitting corrosions in the thin films deposited with 20% N2 flow rate were different.
The mixing enthalpy among the elements in NbTiAlSiZr HEA is large and negative, and HEAs possess slow diffusion effect. Therefore, NbTiAlSiZr HEA films easily form amorphous structure under extreme cooling conditions. The amorphous structure will help to improve the corrosion resistance of the HEA film due to the lack of grain boundary corrosion. In addition, the homogeneous distribution of elements in the HEA film also play an important role to improve corrosion resistance [36]. However, the NbTiAlSiZr HEA film is a Cr-free film and it does not contain corrosion-resistant elements, such as Cr, Co, and Ni, with Ecorr and Epit values lower than those for 304 SS. When a small amount of nitrogen atoms were added into HEAs, some free electrons in HEAs were captured by nitrogen ions. As a result, the free electron concentration decreased, the Ecorr and Epit of NbTiAlSiZrNx HEA films are close to those of 304 SS (Figure 7b). With the further increase of nitrogen content, Ecorr and Epit of NbTiAlSiZrNx HEA films with 20% N2 flow rate were higher than those of 304 SS (Figure 7c). This is due to the fact that the covalent bond between metal and nitrogen is stronger than the metal bond. The short-range order appeared in NbTiAlSiZrNx HEA films when RN further increased to 30%. Ecorr and Epit slightly decreased because the migration of nitrogen atoms broke the homogeneous distribution of the NbTiAlSiZrNx HEA film (Figure 7d). Several corrosion potentials appeared on the polarization curve when RN was larger than 40%, the corrosion occurred on several elements of the HEA films (Figure 7d,f).

5. Conclusions

The design and preparation of the NbTiAlSiZrNx HEA thin film was feasible using fixed radio frequency pulse magnetron sputtering process parameters and time, and under N2 flow rates of 0, 10, 20, 30, 40, and 50% to prepare the NbTiAlSiZrNx HEA thin film on the 304 SS substrate.
When the N2 flow rate increased, the sample hardness with 50% RN was 12.4 GPa, the modulus was 169 GPa, the color was beautiful and varied, roughness was small, but the roughness of the thin film prepared under the conditions of 30% N2 flow rate was relatively high. The thickness of the thin film gradually reduced from 298.8 nm to 200 nm, and the thin films were amorphous.
N2 flow rate increased during the process, the electrochemical corrosion resistance performance of NbTiAlSiZrNx HEA thin film changed in 0.5 mol/L H2SO4 solution. The N2 flow rate of 10% and 30% of the thin film were prone to corrosion more than 304 SS, but its corrosion rate was lower than that of 304 SS. The thin film with N2 flow rate of 20, 40, and 50% was more corrosion-resistant than 304 SS. The passivation stability of NbTiAlSiZrNx HEA was worse than that of 304 SS. The thin film with 40% N2 flow ratio had a high corrosion resistance and the thin film with 30% N2 flow rate had a low corrosion resistance. The corrosion resistance was high, and the film with N2 flow rate of 30% had lower corrosion resistance. Moreover, pitting corrosion occurred in the NbTiAlSiZrNx HEA thin film.

Author Contributions

Writing—original draft preparation, H.W.; writing—review and editing, M.C., Z.C., Q.X., and P.J.; Resources, R.L.; supervision, Y.Z.

Funding

This research was funded by the National Natural Science Foundation of China, grant number 51671020, 5167010608, 51671125 and Natural Science Foundation of Shanghai, grant number 16ZR1412800.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Braic, M.; Braic, V. Characteristics of (TiAlCrNbY)C films deposited by reactive magnetron sputtering. Surf. Coat. Technol. 2010, 204, 2010–2014. [Google Scholar] [CrossRef]
  2. Tsai, C.; Lai, S. Strong amorphization of high-entropy AlBCrSiTi nitrde film. Thin Solid Films 2012, 520, 2613–2618. [Google Scholar] [CrossRef]
  3. Xue, W.; Zhu, Q. Characterization of ceramic coatings fabricated on zirconium alloy by plasma electrolytic oxidation in silicate electrolyte. Mater. Chem. Phys. 2010, 120, 656–660. [Google Scholar] [CrossRef]
  4. Huang, M.; Wang, Y. Corrosion Resistance of Fe–Al/Al2O3 Duplex Coating on Pipeline Steel X80 in Simulated Oil and Gas Well Environment. Surf. Rev. Lett. 2015, 22, 1550045. [Google Scholar] [CrossRef]
  5. Xue, K.; Niu, L. XPS Analysis of Silicon Oxycarbide Formed on the Surface of Rf-sputter Deposited SiC Thin Films. Key Eng. Mater. 2007, 353–358, 1871–1874. [Google Scholar] [CrossRef]
  6. Mondal, A.K.; Kumar, S. Effect of laser surface treatment on corrosion and wear resistance of ACM720 Mg alloy. Surf. Coat. Technol. 2008, 202, 3187–3198. [Google Scholar] [CrossRef]
  7. Hsueh, H.; Shen, W. Effect of nitrogen content and substrate bias on mechanical and corrosion properties of (Al Cr Si Ti Zr)100-xNx high-entropy films. Surf. Coat. Technol. 2012, 206, 4106–4112. [Google Scholar] [CrossRef]
  8. Li, Z. Study on the Design and Preparation of a New Type of Reflective Film with Wide Band Width Angle. Ph.D. Thesis, University of Chinese Academy of Sciences, Beijing, China, 2016. [Google Scholar]
  9. Bertolino, V.; Cavallaro, G. Halloysite nanotubes sandwiched between chitosan layers: Novel bionanocomposites with multilayer structures. New J. Chem. 2018, 42, 8384–8390. [Google Scholar] [CrossRef]
  10. Cicco, D.; Asaee, Z. Use of Nanoparticles for Enhancing the Interlaminar Properties of Fiber-Reinforced Composites and Adhesively Bonded Joints-A Review. Nanomaterials 2017, 7, 360. [Google Scholar] [CrossRef]
  11. Duan, H.; Sun, J. Research progress of coating materials and sputtering targets. In Proceedings of the 2015 Annual Meeting of the Society of Vacuum Society of Guangdong Province, Zhanjiang, China, 26–28 November 2015. [Google Scholar]
  12. Shen, W.; Tsai, M. Effects of substrate bias on the structure and mechanical properties of (Al1.5CrNb0.5Si0.5Ti)Nx coatings. Thin Solid Films 2012, 520, 6183–6188. [Google Scholar] [CrossRef]
  13. Zhang, Y. Amorphous and High-Entropy Alloys; Science Press: Beijing, China, 2010. [Google Scholar]
  14. Murty, B.S.; Yeh, J. High-Entropy Alloys; Elsevier Inc.: Amsterdam, The Netherlands, 2014; pp. 25–35. [Google Scholar]
  15. Feng, X.; Tang, G. Chemical state and phase structure of (TaNbTiW)N films prepared by combinatined magnetron sputtering and PBII. Appl. Surf. Sci. 2013, 280, 388–393. [Google Scholar] [CrossRef]
  16. Michael, C.G. Progress in High Entropy Alloys. JOM 2014, 66, 1964–1965. [Google Scholar] [CrossRef]
  17. Feng, W.; Qi, Y. Effects of Short-Range Order on the Magnetic and Mechanical Properties of FeCoNi(AlSi)x High Entropy Alloys. Metals 2017, 7, 482. [Google Scholar] [CrossRef]
  18. Zhai, S.; Wang, W. Effect of Co and Gd Additions on Microstructures and Properties of FeSiBAlNi High Entropy Alloys. Entropy 2018, 20, 487. [Google Scholar] [CrossRef]
  19. Liu, X.; Yin, H. Microstructure, Mechanical and Tribological Properties of Oxide Dispersion Strengthened High-Entropy Alloys. Materials 2017, 10, 1312. [Google Scholar] [CrossRef]
  20. Klimova, M.; Stepanov, N. Microstructure and Mechanical Properties Evolution of the Al, C-Containing CoCrFeNiMn-Type High-Entropy Alloy during Cold Rolling. Materials 2018, 11, 53. [Google Scholar] [CrossRef]
  21. Cicala, G.; Giordano, D.; Tosto, C.; Filippone, G.; Recca, A.; Blanco, I. Polylactide (PLA) Filaments a Biobased Solution for Additive Manufacturing: Correlating Rheology and Thermomechanical Properties with Printing Quality. Materials 2018, 11, 1191. [Google Scholar] [CrossRef]
  22. Senkov, O.N.; Woodward, C. Microstructure and Propeties of Aluminum-Containing Refractory High-Entropy Alloys. JOM 2014, 66, 2030–2042. [Google Scholar] [CrossRef]
  23. Sheng, W.; Yang, X. Nano-Crystallization of High-Entropy Amorphous NbTiAlSiWxNy Films Prepared by Magnetron Sputtering. Entropy 2016, 18, 226. [Google Scholar] [CrossRef]
  24. Feng, X.; Zhang, J. Stable nanocrystalline NbMoTaW high-entropy alloy thin films with excellent mechanical and electrical propeies. Mater. Lett. 2018, 210, 24–27. [Google Scholar] [CrossRef]
  25. Zhang, S.; Wu, C. Synthesis of Laser High Entropy Alloying Coating on The Surface of Single-element Fe Base Alloy. Acta Metall. Sin. 2014, 50, 555–560. [Google Scholar] [CrossRef]
  26. Li, P.; Chen, J. Research progress of high-entropy alloy coating. Mater. Prot. 2015, 48, 44–46. [Google Scholar] [CrossRef]
  27. Braeckman, B.R.; Boydens, F. High entropy alloy thin films deposited by magnetron sputtering of powder targets. Thin Solid Films 2015, 580, 71–76. [Google Scholar] [CrossRef]
  28. Wang, F.; Liu, H. Advances in ion plating technology. Vacuum 2014, 51, 1–8. [Google Scholar] [CrossRef]
  29. Huang, P.; Yeh, J. Effects of nitrogen content on structure and mechanical properties of multi-element. Surf. Coat. Technol. 2009, 203, 1891–1896. [Google Scholar] [CrossRef]
  30. Chang, S.; Lin, S. Microstructures and mechanical properties of multi-component (AlCrTiZr)NxCy nanocomposite coatings. Thin Solid Films 2011, 519, 4865–4869. [Google Scholar] [CrossRef]
  31. Liu, X. Study on AlxFeCrCoNiCu High-Entropy Alloy Coating for Corrosion Protection of Steel Matrix. Ph.D. Thesis, Institute of technology Dalian, Dalian, China, 2014; pp. 81–100. [Google Scholar]
  32. Sheng, W.; Yang, X. Amorphous phase stability of NbTiAlSiNX high-entropy films. Rare Metal. 2018, 32, 682–689. [Google Scholar] [CrossRef]
  33. Xing, Q.; Xia, S. Mechanical properties and thermal stability of (NbTiAlSiZr)Nx high-entropy ceramic films at high temperatures. J. Mater. Res. 2018, 33, 3347–3354. [Google Scholar] [CrossRef]
  34. Xing, Q.; Ma, J. High-Throughput Screening Solar-Thermal Conversion Films in a Pseudobinary (Cr, Fe, V)-(Ta, W) System. ACS Comb. Sci. 2018, 20, 602–610. [Google Scholar] [CrossRef]
  35. Zhang, Y.; Yan, X. Effects of Nitrogen Content on the Structure and Mechanical Properties of (Al0.5CrFeNiTi0.25)Nx High-Entropy Films by Reactive Sputtering. Entropy 2018, 20, 624. [Google Scholar] [CrossRef]
  36. Gao, L.; Liao, W. Microstructure, Mechanical and Corrosion Behaviors of CoCrFeNiAl0.3 High Entropy Alloy (HEA) Films. Coatings 2017, 7, 156. [Google Scholar] [CrossRef]
  37. Feng, X.; Zhang, Y. Size effects on the mechanical properties of nanocrystalline NbMoTaW refractory high entropy alloy thin films. Int. J. Plast. 2017, 95, 264–277. [Google Scholar] [CrossRef]
Figure 1. SEM images of NbTiAlSiZrNx HEA films’ morphology at: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%.
Figure 1. SEM images of NbTiAlSiZrNx HEA films’ morphology at: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%.
Entropy 21 00396 g001
Figure 2. Changes in the thickness and sputtering deposition rate of NbTiAlSiZrNx HEA films.
Figure 2. Changes in the thickness and sputtering deposition rate of NbTiAlSiZrNx HEA films.
Entropy 21 00396 g002
Figure 3. Surface morphology and color of the NbTiAlSiZrNx HEA films as determined by AFM (a,f) RN = 10%, (b,j) RN = 20%, (c,h) RN = 30%, (d,i) RN = 40%, and (e,g) RN = 50%.
Figure 3. Surface morphology and color of the NbTiAlSiZrNx HEA films as determined by AFM (a,f) RN = 10%, (b,j) RN = 20%, (c,h) RN = 30%, (d,i) RN = 40%, and (e,g) RN = 50%.
Entropy 21 00396 g003
Figure 4. Changes in the roughness values of NbTiAlSiZrNx HEA films.
Figure 4. Changes in the roughness values of NbTiAlSiZrNx HEA films.
Entropy 21 00396 g004
Figure 5. (a) Load-Displacement curves of the NbTiAlSiZrNx HEA films; (b) changes in the loading energy of the NbTiAlSiZrNx HEA films; (c) hardness–displacement curves of NbTiAlSiZrNx HEA films; and (d) changes in the hardness and modulus values of NbTiAlSiZrNx HEA films.
Figure 5. (a) Load-Displacement curves of the NbTiAlSiZrNx HEA films; (b) changes in the loading energy of the NbTiAlSiZrNx HEA films; (c) hardness–displacement curves of NbTiAlSiZrNx HEA films; and (d) changes in the hardness and modulus values of NbTiAlSiZrNx HEA films.
Entropy 21 00396 g005
Figure 6. SEM images before and after corrosion of NbTiAlSiZrNx high-entropy films in the 0.5 mol/L H2SO4 solution. Before: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%. After: (f) RN = 10%, (g) RN = 20%, (h) RN = 30%, (i) RN = 40%, and (j) RN = 50%.
Figure 6. SEM images before and after corrosion of NbTiAlSiZrNx high-entropy films in the 0.5 mol/L H2SO4 solution. Before: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%. After: (f) RN = 10%, (g) RN = 20%, (h) RN = 30%, (i) RN = 40%, and (j) RN = 50%.
Entropy 21 00396 g006aEntropy 21 00396 g006b
Figure 7. Dynamic potential polarization curves of NbTiAlSiZrNx high-entropy films and 304 stainless steel in 0.5 mol/L H2SO4 solution. (a) all sample, (b) RN = 10%, (c) RN = 20%, (d) RN = 30%, (e) RN = 40%, and (f) RN = 50%.
Figure 7. Dynamic potential polarization curves of NbTiAlSiZrNx high-entropy films and 304 stainless steel in 0.5 mol/L H2SO4 solution. (a) all sample, (b) RN = 10%, (c) RN = 20%, (d) RN = 30%, (e) RN = 40%, and (f) RN = 50%.
Entropy 21 00396 g007
Figure 8. Relationship between the self-corrosion potential and the current of NbTiAlSiZrNx HEA films with the ratio of N2 flow.
Figure 8. Relationship between the self-corrosion potential and the current of NbTiAlSiZrNx HEA films with the ratio of N2 flow.
Entropy 21 00396 g008
Figure 9. TEM images of NbTiAlSiZrNx thin films at: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%.
Figure 9. TEM images of NbTiAlSiZrNx thin films at: (a) RN = 10%, (b) RN = 20%, (c) RN = 30%, (d) RN = 40%, and (e) RN = 50%.
Entropy 21 00396 g009
Figure 10. X-ray diffraction (XRD) patterns of NbTiAlSiZrNx thin films.
Figure 10. X-ray diffraction (XRD) patterns of NbTiAlSiZrNx thin films.
Entropy 21 00396 g010
Table 1. Atomic radii (ri) of the constituent elements.
Table 1. Atomic radii (ri) of the constituent elements.
ElementNbTiAlSiZr
ri1.481.451.431.341.60
Table 2. Elemental components of the NbTiAlSiZr high entropy alloy (the atomic percent content).
Table 2. Elemental components of the NbTiAlSiZr high entropy alloy (the atomic percent content).
ElementNbTiAlSiZr
Nominal content/at. %2020202020
Actual content/at. %20.5619.5221.0019.3819.54
Note: the test mode was the EDX area scan.

Share and Cite

MDPI and ACS Style

Xing, Q.; Wang, H.; Chen, M.; Chen, Z.; Li, R.; Jin, P.; Zhang, Y. Mechanical Properties and Corrosion Resistance of NbTiAlSiZrNx High-Entropy Films Prepared by RF Magnetron Sputtering. Entropy 2019, 21, 396. https://doi.org/10.3390/e21040396

AMA Style

Xing Q, Wang H, Chen M, Chen Z, Li R, Jin P, Zhang Y. Mechanical Properties and Corrosion Resistance of NbTiAlSiZrNx High-Entropy Films Prepared by RF Magnetron Sputtering. Entropy. 2019; 21(4):396. https://doi.org/10.3390/e21040396

Chicago/Turabian Style

Xing, Qiuwei, Haijiang Wang, Mingbiao Chen, Zhaoyun Chen, Rongbin Li, Peipeng Jin, and Yong Zhang. 2019. "Mechanical Properties and Corrosion Resistance of NbTiAlSiZrNx High-Entropy Films Prepared by RF Magnetron Sputtering" Entropy 21, no. 4: 396. https://doi.org/10.3390/e21040396

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop